RAGM10
- Reinforced with 50% Glass Fiber & Mineral Fillers
- Product Benefits: High Rigidity with Good-looking Surface, High Dimensional Stability, Low Moisture Absorption
- Certificate:RoHS、REACH
- Scroll down to download PDF version
Technical Properties
Swipe Right to View Full Details
| Properties | Test Method | Units | Conditions | Value |
|---|---|---|---|---|
| Density | ISO 1183 | g/cm3 | Dry | 1.58 |
| Tensile strength at break | ISO 527 (50mm/min) |
Mpa | Dry Cond. |
240 210 |
| Flexural strength | ISO 178 | Mpa | Dry Cond. |
400 330 |
| Elongation at break | ISO 527 (50mm/min) |
% | Dry Cond. |
2.2 2.5 |
| Impact strength | ISO 180-1C Charpy,23℃ |
Kj/㎡ | Dry Cond. |
85 82 |
| Impact strength | ISO 180-1C Charpy,-30℃ |
Kj/㎡ | Dry Cond. |
75 74 |
| Notched impact strength | ISO 180-1A Charpy,23℃ |
Kj/㎡ | Dry Cond. |
14 14 |
| Notched impact strength | ISO 180-1A Charpy,-30℃ |
Kj/㎡ | Dry Cond. |
14 13 |
| Ball indentation hardness | ISO | Mpa | Dry Cond. |
310 285 |
| Melting point | ISO 3146C DSC | ℃ | Dry | 258 |
| Heat deflection temperature HDT/A | ISO 75 0.45 Mpa | ℃ | Dry | 235 |
| Heat deflection temperature HDT/B | ISO 75 1.8MPa |
℃ | Dry | 200 |
Download file